## Querying This Documentation
This site has an agentic ask interface you may use to query the documentation dynamically by asking a question.

Perform an HTTP GET request on the following URL with the `ask` and `goal` query parameters:

```
GET https://docs.hackerfabiitb.org/index.md?ask=<question>&goal=<user_goal>
```

`ask` is the immediate question: it should be specific, self-contained, and written in natural language.
`goal` is what the user is ultimately trying to achieve, the reason they need the answer. Sharing it helps GitBook give you a better, more relevant answer. A goal is most helpful when it describes the outcome the user wants rather than restating the question. For example, with `ask=how do I create an API token`, a goal like `automate deployments from our CI pipeline` lets GitBook tailor the answer to that use case.

The response will contain a direct answer to the question and relevant excerpts and sources from the documentation.

---

# HackerFab IITB Docs

Homepage

Welcome to the technical documentation of HackerFab IITB, India's first student-build semiconductor fab for education!

For information about the team, getting in contact, and recruitment, see our website: <https://hackerfabiitb.org/>

We are gradually documenting our tools, please be patient if a page looks incomplete! Meanwhile, watch our zero-to-one video which explains everything you need to know about setting up a HackerFab:

{% embed url="<https://youtu.be/q6RficsT3f4>" %}

We have extensive discussions on Discord: <https://discord.gg/FNUgVRxmef> . For example, for doubts about our litho system, post on the `#litho-v1` channel.

We stand on the shoulders of the rest of the HackerFab community, which is thoroughly documented at <https://docs.hackerfab.org/>

Many thanks to Gitbook for supporting educational projects like ours in the form of the Gitbook Community Edition!


# litho-v1

A direct-write photolithography system with 5um line/space under INR 2,00,000

Our lithography system is based HackerFab CMU's Litho v2.1+ (which is their latest as of September 2026): <https://docs.hackerfab.org/home/fab-toolkit/patterning/lithography-stepper-v2.1+-build>

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FTatzcWQIgYJ5eW7vtsbn%2Flitho_setup.jpg?alt=media&amp;token=ad1a9be5-2de9-4b78-984e-f8101ff093f3" alt=""><figcaption><p>litho-v1 setup with litho-control software in yellow room</p></figcaption></figure>

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FGh2qKAtmdNy5PN30ZIv1%2Fnew_res_test.jpg?alt=media&amp;token=380e5cac-4c09-473c-b674-f6ebbe033c9f" alt=""><figcaption><p>3 micron line / 7 micron space features</p></figcaption></figure>

## Intro

Lithography means writing patterns into stone (Greek: lithos: stone, graphy: to write). Lithography is used in microfabrication to create patterns of a circuit on silicon.\
Photolithography exposes the pattern of light onto a thin film of photoresist coated on the sample. For positive photoresist, the regions of resist exposed to light undergo a chemical change which makes them soluble in a developer.

Our photolithography system uses a DLP projector with a UV LED modification.

## Why DLP?

Masked lithography shines blanket light through a hard mask consisting of transparent and opaque regions. This is used for high-throughput, high-resolution patterning for mass-manufacture of Integrated Circuits. The mask is expensive and slow to make, hence unsuitable for rapid prototyping at a student level.\
The hard mask itself is made using a maskless lithography system, which can be of 2 types:

1. Writer: a beam of photons (laser writing) or electrons (EBL: electron beam lithography) is scanned across the sample. Extremely high-resolution (<10nm for EBL), but low-throughput (slow). Used in research. Requires extremely precise motion stages to deflect the beam.
2. DMD: uses a DMD chip (<https://en.wikipedia.org/wiki/Digital_micromirror_device>) to selectively block or reflect regions of light from a light source. Does not need beam deflection motion stages, and is much faster than writers because it exposes a large (approx 10mm wide before demagnification) area in a single exposure. However, its resolution is limited by the DMD pixel pitch. It is the perfect compromise for DIY litho: low-cost albeit low-throughput and low-resolution

The DMD chip itself can be found in consumer DLP (<https://en.wikipedia.org/wiki/Digital_light_processing>) projectors. The DLP projector uses 3 LED light sources (Red, Green, Blue) illuminating the mirror array (DMD) to form the image. This enables swapping the blue LED for a 405nm UV led, which is suitable for exposing photoresist. **This would not be possible in a regular LCD projector**, as each of the millions of pixels has individual R,G,B leds, which cannot be swapped out for UV.

The silicon microfabrication revolution enabled cheap production of MEMS devices, which in turn makes our lithography system inexpensive!

## Optical Specifications

LED Wavelength: 405nm\
Lens NA: 0.25\
DMD pixel pitch: TODO

## System Performance

line/space for nominal 5um/5um line array: 4um/6um\
isolated line widths: TODO\
XYZ stage repeatability, tiling error, overlay error: TODO

## Bill of Materials

INR 2 Lakh Budget

<table><thead><tr><th>Item Name</th><th>Cost (INR) as of August 2026</th><th data-type="content-ref"></th></tr></thead><tbody><tr><td>TI DLP Evaluation Module (DLPDLCR471TPEVM) from Mouser</td><td>1,10,000</td><td><a href="https://www.mouser.in/en/ProductDetail/Texas-Instruments/DLPDLCR471TPEVM?qs=DRkmTr78QAQsT6dpWa8zKg%3D%3D">https://www.mouser.in/en/ProductDetail/Texas-Instruments/DLPDLCR471TPEVM?qs=DRkmTr78QAQsT6dpWa8zKg%3D%3D</a></td></tr><tr><td>Edmund Optics Beamsplitter (25 x 25mm, 25R/75T, AR Coated)</td><td>6,357</td><td><a href="https://www.edmundoptics.in/p/25-x-25mm-25R75T-AR-Coated-Plate-Beamsplitter/45377">https://www.edmundoptics.in/p/25-x-25mm-25R75T-AR-Coated-Plate-Beamsplitter/45377</a></td></tr><tr><td>Edmund Optics 10X DIN Plan Commercial Grade Objective</td><td>20,178</td><td><a href="https://www.edmundoptics.in/p/10x-din-plan-commercial-grade-objective/5386">https://www.edmundoptics.in/p/10x-din-plan-commercial-grade-objective/5386</a></td></tr><tr><td>Basler ace scientific camera</td><td>~10,000</td><td><a href="https://www.baslerweb.com/en-in/shop/aca1920-40um/">https://www.baslerweb.com/en-in/shop/aca1920-40um/</a></td></tr><tr><td>XYZ Stage 40mm. (TODO ADD 60mm one here)</td><td>~7,000</td><td><a href="https://www.alibaba.com/product-detail/Diacion-Manual-XYZ-3-Axis-Linear_1601564564707.html?spm=a2700.prosearch.normal_offer.d_title.7cf967afK3ag89&#x26;priceId=a1142dd115ea46f6b0842707485dab9c">https://www.alibaba.com/product-detail/Diacion-Manual-XYZ-3-Axis-Linear_1601564564707.html?spm=a2700.prosearch.normal_offer.d_title.7cf967afK3ag89&#x26;priceId=a1142dd115ea46f6b0842707485dab9c</a></td></tr><tr><td>NEMA 28 Stepper x 3</td><td>2,100</td><td><a href="https://amzn.in/d/00fimvk9">https://amzn.in/d/00fimvk9</a></td></tr><tr><td>UV LEDs from ktron</td><td>100</td><td><a href="https://www.ktron.in/product/uv-led-5w-410-420nm-1200ma-smd3535/">https://www.ktron.in/product/uv-led-5w-410-420nm-1200ma-smd3535/</a></td></tr><tr><td>Mounts: Metal &#x26; Machining</td><td>TODO</td><td><a href="https://github.com/hackerfabiitb/litho_machining_m27x1.5">https://github.com/hackerfabiitb/litho_machining_m27x1.5</a></td></tr></tbody></table>

## Software

### &#x20;Prerequisites

| Sr No | Software Name  | Purpose                                            | Instructions                                                                       | Link                                                                                        |
| ----- | -------------- | -------------------------------------------------- | ---------------------------------------------------------------------------------- | ------------------------------------------------------------------------------------------- |
| 1     | Basler Pylon   | Receiving video feed from industrial camera        | Download the latest version of Pylon (the software suite, not the redistributable) | <https://www.baslerweb.com/en/downloads/software/?downloadCategory.values.label.data=pylon> |
| 2     | TI DLP EVM GUI | Controlling DLP LED intensities                    | DLPDLC-GUI, NOT Lightcrafter                                                       | <https://www.ti.com/tool/DLPDLC-GUI>                                                        |
| 3     | GIMP           | Open-source image editor for creating masks        |                                                                                    | <https://www.gimp.org/downloads/>                                                           |
| 4     | OBS Studio     | viewing the video feed being sent to the projector |                                                                                    | <https://obsproject.com/download>                                                           |

### litho-control

`litho-control` is a software developed by us to control the projector, camera and XYZ stage in one window. Install it from <https://github.com/hackerfabiitb/litho-control>

Features:

1. autofocus
2. exposure sweeps
3. Scan for widefield images(step, autofocus, take image, repeat)
4. optical tracking to track in-camera features during stage movement, to calibrate stage performance.

## Chemicals Used

1. S1813 PPR: Positive Photoresist: exposed parts are soluble in developer. [Datasheet](https://drive.google.com/file/d/1xYIi1hyWTzFgmqcuzrqd_HlrwxEy8HMW/view?usp=drive_link), [MSDS 1](https://drive.google.com/file/d/1EmSJbKPpif73l_fudvb6x7Dx4e-fZoJc/view?usp=drive_link), [MSDS 2](https://drive.google.com/file/d/1jNVW-7bWbhX3y3jYUYZ0rI_DoDHn2GJi/view?usp=drive_link)
2. LOR 3b: lift-off resist used for removing un-patterned metal after sputtering. Not photosensitive, but used to provide undercut (see[Liftoff and Undercut in Deposition](https://docs.hackerfabiitb.org/fab-basics/liftoff-and-undercut-in-deposition)). TODO Datasheet, MSDS
3. Mf319 Developer: removes LOR and exposed PPR. [Datasheet](https://drive.google.com/file/d/1XRJLITyVZ61BJQAi83fC5ZQ2qnj0IHLI/view?usp=drive_link), [MSDS](https://drive.google.com/file/d/1mUCmngaEArfdS0SmwkyfwTIn1UmCWHU0/view?usp=drive_link)
4. PG Remover: removes resists ignoring exposure. [Datasheet](https://drive.google.com/file/d/1LLKt0cq4torESFUye8tevUG-2PJ9fTeg/view?usp=drive_link), [MSDS](https://drive.google.com/file/d/1CHMThWx8GCKCOkcU-4_TkZDemfF-qgW7/view?usp=drive_link)

## Notes

Post-exposure bake has not been tested. It may improve development.&#x20;

Exposure dose = 140mJ/cm^2 is the dose optimized by IITBNF. We don't have capability to measure intensity yet. See [#led-current-mapping](#led-current-mapping "mention")

The optimal dose and develop varies with resist age, temperature, humidity etc. A reasonable range is 120-160mJ/cm^2 and 15s to 40s respectively.

#### LED current mapping

As discovered by TODO on the HackerFab Discord, the current shown in the software maps to actual LED milliamps by TODO formula


# SOP

Systematic operating procedure for litho-v1

NOTE: read [litho-v1](https://docs.hackerfabiitb.org/tools/litho-v1) first to understand the litho system.

## 1. Wafer Prep

Proceed to the next step if doing litho on an existing sample, eg on a sputtered film, or doing 2nd level litho. Else:

1. Cut a wafer piece with diamond scribe
2. Clean with acetone, then IPA, then dry with N2.

## 2. Spincoating

Use PPR\_spin+bake when doing isolated litho runs, or for etching.

Do LOR\_spin+bake then PPR\_spin+bake when doing litho then sputtering then liftoff.

### PPR\_spin+bake

| Sr. No. | Process           | Step    | Parameters                                              |
| ------- | ----------------- | ------- | ------------------------------------------------------- |
| 1       | PPR spincoating   | Step-1  | <p>Time = 10 s<br>RPM = 500<br>Acceleration = 250</p>   |
|         |                   | Step-2  | <p>Time = 45 s<br>RPM = 4000<br>Acceleration = 2000</p> |
|         |                   | Step-3  | <p>Time = 10 s<br>RPM = 0<br>Acceleration = 500</p>     |
| 2       | Pre-exposure Bake | Heating | <p>Time = 3 min<br>Temperature = 90 °C</p>              |

### LOR\_spin+bake

| Sr. No. | Process           | Step    | Parameters                                              |
| ------- | ----------------- | ------- | ------------------------------------------------------- |
| 1       | LOR spincoating   | Step-1  | <p>Time = 10 s<br>RPM = 500<br>Acceleration = 250</p>   |
|         |                   | Step-2  | <p>Time = 45 s<br>RPM = 4000<br>Acceleration = 2000</p> |
|         |                   | Step-3  | <p>Time = 10 s<br>RPM = 0<br>Acceleration = 500</p>     |
| 2       | Pre-exposure Bake | Heating | <p>Time = 5 min<br>Temperature = 150 °C</p>             |

### Dispensing Photoresist

1. **Turn on yellow lights and turn off white lights**
2. Take out S1813 photoresist from fridge and keep it out to reach room temperature
3. Set hot plate to recipe temperature and wait for it to stabilize.

The above steps take time so do them beforehand. Then:

1. Open spincoater lid. Replace the Al foil if it is dirty.
2. Place the sample centred on the O-ring.&#x20;
3. Put new tip on $$100\mu L$$ micropipette
4. Set it to $$100\mu L$$ . This is sufficient for even a 2 inch wafer.
5. Remove the Al foil and open the cap of the resist.
6. Press the pipette plunger. Dip only the tip of the pipette into the liquid. release the plunger
7. Move the tip over the sample. As you dispense move the tip around so the droplets cover the entire wafer
8. Press the slider to release the tip into a garbage bag.
9. Close the spincoater lid.
10. Start the preloaded recipe.
11. Bake according to the recipe. Keep a petri dish over the sample to prevent dust falling.
12. Lower the litho chuck in software (see below)
13. place the sample on the litho chuck

See <https://youtu.be/Jfqafjt4q6U> for how to use a pipette properly.

## 3. Litho

### Startup

1. Turn on the PC and monitor
2. Turn on the XYZ stage power supply
3. Plug in the camera USB cable.
4. Turn on the projector power supply mains
5. Open the DLP EVM GUI software, go to Display > Dynamic black > turn red on and drag the slider to the lowest power (101)
6. Turn on the LEDs switch on the projector PCB. this should turn on all 3 LEDs, which you can see glowing. If not, see [#debugging](#debugging "mention")
7. Immediately click "Set" in the software which keeps only the red LED on\
   **NOTE: do not keep the UV LED on for extended periods of time, it will burn.**
8. Open vscode in `Desktop\litho-control` , open the terminal, and run `.\ui\start.ps1` . Also keep claude code window in vscode open.

### litho-control software

1. Check that the projector, camera and Arduino all show connected
2. Focusing
   1. Click "go to focus" to move to a previously saved focus.
   2. Else, click autofocus with a suitable range and step size.
   3. Else, click the checker button to project a pattern for focusing, and move Z in steps of 500 to 100 to 10 to home in on the focus.
3. Click the TODO button to crop the camera view to the exposure field.

Use "optical tracking" to track features as the stage moves.

Run "Scan" to move the stage and get a wide-field scan.

### Exposure

Ask claude code to run an exposure sweep, which moves and exposes the same pattern for different durations.

There are pre-existing resolution tests in the `patterns` folder. Use claude code for making new resolution tests or custom text patterns.

Good exposure time is around 90s. Sweep from 30s to 120s.

## Development

1. Fill developer in a petri dish, and DI water in a beaker.
2. Dip the wafer in the developer for 20s, keeping it held with tweezers throughout.
3. Immediately immerse it in water and move it gently, to flush the developer out.
4. Dry with N2. The pattern should appear as a small rectangular mark on the wafer.
5. Put under microscope, or use the Scan feature of litho, to inspect the pattern.
6. Repeat from step 2, developing in 10s increments.

See [Litho performance](https://docs.hackerfabiitb.org/fab-basics/litho-performance) for what a "good" exposure+development should look like.

**Remember to send developed images on Discord on the #litho-v1 channel before shutdown.**

The table of images formed from sweeping exposure and development on a give sample is called the **dose matrix.**

## Shutdown

(reverse order of [#startup](#startup "mention"))

1. close litho-control software and DLP EVM GUI software
2. turn off the LED switch and mains of the projector
3. unplug the camera USB cable to prevent overheating
4. turn off the XYZ stage power supply.

## Projector Debugging

Debug > USB connection

Unplug, replug usb cable

remove HDMI cable

check Device Manager

TODO

***

Note: these recipes are based on the ones developed at IITBNF (<https://www.iitbnf.iitb.ac.in/>)


# XYZ Stage

Vacuum Chuck CAD: <https://cad.onshape.com/documents/505a9714dd109f13d4455c6e/w/5c8d0a032a300181db2a2d58/e/852fab0c6cae68c62e8e1a30?renderMode=0&uiState=6a146d61a0c436cac2711f6b>


# sputter-v2

This is the official IITB documentation for the sputter

***

### Table of Contents

1. Introduction
2. What is a Sputter Coater? How does it work?
3. Bill of Materials (BOM)
4. Resources
5. Safety
6. Subsystem Build Instructions
   * Power Supply
   * Vacuum System
   * Chamber
   * Magnetron
   * Gas Flow System
7. Standard Operating Procedure (SOP)
8. Startup / Shutdown Checklists
9. Automation
10. Software
11. Improvements
12. Troubleshooting & Failure Modes
13. Glossary
14. India-Specific Sourcing Notes
15. To-Do / Missing Content
16. Revision History

***

### Introduction

This document describes the design, construction, and safe operation of a DIY magnetron sputter coater built primarily from salvaged and locally available components (with some imported fittings). The system is intended for depositing thin metal films onto substrates under vacuum using DC magnetron sputtering with argon process gas.

**Goals of this documentation**

* Enable a competent person with basic electronics, machining, and vacuum experience to rebuild or maintain the system.
* Provide sufficient safety information so the system can be operated without external assistance once built.
* Serve as the single source of truth for the project (GitBook / internal wiki).

**Audience**

* Makers, student teams, and small research groups with access to a workshop and basic high-voltage / vacuum safety training.
* Not a commercial product manual. Treat every high-voltage and vacuum section with extreme caution.

***

### What is a Sputter Coater? How does it work?

Sputtering is a Physical Vapor Deposition (PVD) technique used to deposit thin films of material onto a substrate.

**Basic process**

1. A vacuum chamber is evacuated to a low base pressure (typically 10⁻⁵ – 10⁻⁶ mbar or better) to remove residual air and water vapor.
2. An inert process gas (almost always argon) is introduced and the pressure is stabilized in the 10⁻³ – 10⁻¹ mbar range.
3. A high negative voltage (typically –300 V to –800 V or higher) is applied to a target made of the material to be deposited (the cathode). The chamber walls or a separate anode are at ground.
4. The electric field ionizes some of the argon atoms, creating a plasma (visible as a characteristic glow).
5. Positive argon ions (Ar⁺) are accelerated toward the negatively biased target and strike it with high kinetic energy.
6. Momentum transfer ejects atoms from the target surface (“sputtering”). These neutral atoms travel through the chamber and condense on the substrate, forming a thin film.

**Why “magnetron” sputtering?**\
In a simple diode sputterer the plasma density is low and deposition rates are slow. A magnetron places permanent magnets behind the target so that the magnetic field is parallel to the target surface (usually in a closed loop / “racetrack”). Electrons are trapped in helical paths near the target by the **E × B** drift. This dramatically increases the ionization probability of argon, producing a dense plasma localized just above the target. Result: higher deposition rates at lower pressures and lower voltages, with less substrate heating.

**Key operating regimes in this build**

* Plasma strike pressure: \~0.1 mbar
* Typical sputtering pressure: 0.01 – 0.001 mbar
* Pressure is maintained dynamically: turbo pump runs continuously while argon flow is adjusted via the mass-flow controller (MFC).

**Placeholder — Performance numbers**\
*\[Add measured base pressure, typical deposition rates for common targets (Au, Ag, Cu, etc.), and any film characterization data once available.]*

***

### Bill of Materials (BOM)

> **Placeholder section — Master table still incomplete.**\
> Populate the table below with every major component. Include quantity, approximate cost (INR preferred), source/link, and notes.&#x20;

| Subsystem | Component                                                | Qty | Approx. Cost (INR) | Source / Notes                        | Status |
| --------- | -------------------------------------------------------- | --- | ------------------ | ------------------------------------- | ------ |
| Vacuum    | Rotary vane pump                                         | 1   | \~50,000           | Local vacuum equipment supplier       | Known  |
| Vacuum    | Turbomolecular pump                                      | 1   | TBD                |                                       | TBD    |
| Vacuum    | Pirani gauge head + controller                           | 1   | TBD                | KF16                                  | TBD    |
| Vacuum    | Penning gauge head + controller                          | 1   | TBD                | KF25                                  | TBD    |
| Vacuum    | KF / ISO / CF fittings, adapters, O-rings, Viton gaskets | —   | TBD                | Various                               | TBD    |
| Chamber   | SS cylinder + flanges                                    | 1   | TBD                | Local steel vendor + laser cutting    | TBD    |
| Chamber   | Top & bottom plates                                      | 2   | TBD                |                                       | TBD    |
| Chamber   | Viewport glass + flange                                  | 1   | TBD                |                                       | TBD    |
| Chamber   | PEEK screws                                              | set | TBD                | Non-conductive top-plate mounting     | TBD    |
| Power     | Variac (0–230 V)                                         | 1   | TBD                |                                       | TBD    |
| Power     | Microwave oven transformer                               | 1+  | Salvaged           | Local appliance repair shops (Mumbai) | Known  |
| Power     | HV diodes + capacitor                                    | —   | Salvaged / order   | Microwave rated                       | TBD    |
| Power     | HV-rated gloves (≥1000 V)                                | 1   | TBD                |                                       | TBD    |
| Magnetron | Mild steel plate (nickel plated)                         | 1   | TBD                | Electroless Ni plating                | TBD    |
| Magnetron | Magnets, cooling if used                                 | —   | TBD                | Follow CMU geometry                   | TBD    |
| Gas       | Argon cylinder + regulator                               | 1   | TBD                |                                       | TBD    |
| Gas       | Mass Flow Controller (MFC)                               | 1   | TBD                | Second-hand (eBay etc.) preferred     | TBD    |
| Gas       | VCR / NPT / KF converters + gaskets                      | —   | TBD                | Often imported or machined            | TBD    |
| Misc      | High-voltage wiring, grounding plate, enclosure          | —   | TBD                |                                       | TBD    |

**Placeholder — Full BOM table**\
*\[Complete the table with exact part numbers, links, lead times, and total estimated budget.]*

***

### Resources

* **Magnetron design reference**: Carnegie Mellon University (CMU) published sputter documentation\
  **Placeholder link** — *\[Insert actual CMU magnetron / sputter documentation URL once confirmed.]*
* Vacuum fundamentals textbook referenced in notes as “Fifer”\
  **Placeholder** — *\[Confirm exact title/author. Common alternatives: “Foundations of Vacuum Science and Technology” (Laﬀerty), Leybold “Fundamentals of Vacuum Technology”, or Berman “Vacuum Engineering Calculations”.]*
* Swagelok fitting selection guides and videos (search “Swagelok VCR”, “Swagelok KF”).
* O-ring groove design: ISO standards for vacuum O-ring grooves (search “ISO vacuum O-ring groove design”).
* Flange standards: KF/NW, ISO-K, ISO-F, CF (ConFlat) comparison charts (many free PDFs from vacuum component vendors).
* MFC gas conversion factors: Brooks Instrument, MKS, or equivalent manufacturer tables (Argon GCF ≈ 1.39–1.40 relative to N₂).

**Placeholder — Additional links**\
*\[Add direct links to specific YouTube videos of the power-supply build, Swagelok tutorials, and any internal photos/diagrams once uploaded.]*

***

### Safety

High voltage, vacuum, and pressurized gas are all present. Treat all three with equal seriousness. **A single careless action can be fatal or destroy expensive components.**

#### High Voltage

* Always wear high-voltage-rated gloves (rated for at least 1000 V) when working on or near the power-supply section.
* Never touch live components. Assume everything is live until proven otherwise with a multimeter.
* Before handling any capacitor, **discharge it** by shorting its terminals with insulated high-voltage-rated tools, then verify zero voltage with a digital multimeter (DMM).
* Be extremely careful about accidental shorts. Keep the work area clear of conductive objects.
* Mount the variac and enclosure to a common grounded metal plate. Connect the AC plug ground pin to the enclosure. Ground one side of the high-voltage capacitor to the enclosure body.

#### Vacuum / Pressure

* Prefer metal chambers. Avoid glass jars for anything beyond early low-pressure prototyping; if used, enclose them in a protective housing against implosion.
* **Hard cutoff: treat 1 mbar as the absolute maximum pressure while the turbo pump or Penning gauge is operating.** If pressure is rising toward or above this value, stop argon flow immediately.
* Never vent the chamber to atmosphere while the turbomolecular pump or Penning gauge is on.
* The Penning gauge must **only** be switched on after the Pirani gauge indicates a safe low pressure. Powering a Penning gauge at high pressure will cause internal arcing and permanent damage.\
  **Exact interlock threshold (TBD)** — typical industry practice is often around 10⁻² mbar or lower; confirm with the specific gauge controller manual and mark the value here once verified.
* Turbo pump inlet path must be short and direct (see Vacuum System section).

#### Gas Handling

* Argon is inert but can displace oxygen in a confined space. Ensure good ventilation.
* Always use the correct regulators, fittings, and single-use VCR gaskets.
* Double-check male/female compatibility at every joint.

#### General

* Only trained personnel should operate the system.
* Keep a multimeter, HV-rated tools, and a fire extinguisher appropriate for electrical fires nearby.
* **Placeholder — Lab / institutional requirements**\
  *\[Add any required electrical safety sign-off, vacuum safety training, or local regulations that apply in your institution.]*

***

### Subsystem Build Instructions

#### Power Supply

Components can be salvaged from microwave ovens with strict precautions.

**Precautions when salvaging from a microwave**

1. Discharge the high-voltage capacitor completely before touching anything. Short the terminals with insulated tools, then verify zero volts with a DMM. Wear ≥1000 V rated gloves.
2. The magnetron tube itself often has a beryllium-oxide ceramic coating that is toxic if scraped or powdered. Handle carefully; do not drop or abrade it.

**Circuit topology**\
Variac (0–230 V AC) → Microwave oven transformer (step-up ≈ ×10) → Full-wave rectifier (HV diodes + capacitor) → High-voltage DC output to magnetron cathode.

* **Variac**: Throttles input voltage, giving roughly 0–2 kV AC at the secondary of the microwave transformer.
* **Microwave transformer identification**: Primary has lower DC resistance and usually two accessible terminals. Secondary has higher resistance; one end is often the core / ground reference. Accessing the secondary terminal may require polishing the casing or using a mounting hole.
* **Rectifier**: Use microwave-rated HV diodes and capacitor. A single microwave usually supplies only one diode — order spares. Transformers are harder to source; appliance repair shops that service microwaves are a good local source (successfully used in Mumbai).
* **Grounding**: Mount variac and enclosure to the same metal plate so the enclosure is grounded. Ground one terminal of the capacitor to the enclosure. AC ground pin → enclosure.

**Placeholders**

* *\[Circuit diagram: variac → transformer → rectifier → grounding.]*
* *\[Photos of each subsection and of the open-table prototype, including any relevant incident notes.]*
* *\[Link to all related build videos.]*
* *\[Photo / product link for the exact HV gloves used.]*

#### Vacuum System

**Pump configuration**\
Rotary vane pump → hose → turbomolecular pump → chamber.\
The rotary pump roughs the system through the turbo; once pressure is low enough the turbo is started.

> Note: This is a non-standard arrangement. In many professional systems the main chamber stays under continuous high vacuum and samples are introduced via a load-lock. The present design cannot hold the chamber at low vacuum independently of the turbo.

**Two flow regimes**

1. Viscous / continuum regime — molecules collide with each other; rotary pump is effective.
2. Molecular flow regime — molecules travel independently; turbo pump is required.

**Turbo pump plumbing**\
The turbo does not “suck”; its blades physically impart momentum to molecules. Keep the path from chamber to turbo inlet short, direct, and preferably straight or gently curved. Avoid long or convoluted hoses.

**Sealing principles**

* Two flat surfaces always have microscopic gaps → a soft gasket (Viton O-ring or flat gasket) fills them under compression.
* **KF (NW) flanges**: O-ring + clamp.
* To seal a component to a flat plate: machine a groove or use a gasket + perimeter screws that provide even compression.
* **ISO flanges**: ISO-K (clamp) and ISO-F (bolt).
* **CF (ConFlat)**: knife-edge + copper gasket (metal seal).

In this build an ISO-to-CF adapter was used; a Viton gasket was cut to sit on the CF knife-edge.\
**Lesson learned**: An ISO-K to ISO-F adapter would have been cleaner and fully Viton-compatible.

**Gauges**

* Pirani gauge (accurate roughly down to 10⁻³ mbar) — KF16 in this build (reducer used).
* Penning (cold-cathode) gauge for lower pressures — KF25.
* Each gauge needs its own head **and** controller.
* **Critical interlock**: Penning only after Pirani reads safely low. Exact threshold still TBD — mark it here once measured / confirmed from the gauge manuals.

**Placeholders**

* *\[Diagram of short turbo-to-chamber geometry.]*
* *\[Photos of KF assembly, O-ring vs gasket, KF16/KF25.]*
* *\[Exact Penning interlock pressure.]*
* *\[Verification of Viton-on-CF description and of the exhaust-line wording.]*

#### Chamber

Three main parts: top plate, cylindrical body, bottom plate.

**Material & thickness**

* Stainless steel preferred, minimum 8–10 mm wall thickness (conservative; no rigorous calculation was performed).
* Top/bottom plates may be steel or aluminum if using gasketed bolted joints. Welded flanges require matching steel.

**Fabrication philosophy**\
No welds on any vacuum-sealing surface. All welds are purely structural and located on the outside of the cylinder side-wall.

Body fabrication sequence:

1. Cut SS pipe to length (ID sized for required working volume).
2. Laser-cut or CNC flanges (rings) matching the pipe OD with margin for screw holes.
3. Weld flanges to the **outside** of the cylinder side walls only.
4. Mirror-polish all vacuum-facing surfaces (inner walls + flange faces) to reduce outgassing.

Top & bottom plate sealing:

* Matching bolt circles + O-ring groove slightly inboard of the bolts, just outside the chamber ID. Follow ISO O-ring groove guidelines for stretch and compression.

**Viewport**\
Mounted through the top plate (side viewport impossible without sealing welds).\
Sequence: groove → O-ring → glass → clamping flange → bolts.

**Electrical isolation**\
Top plate and body are at different potentials → use non-conductive **PEEK screws**.\
All mounting holes are blind tapped holes (through-holes would leak). Vented screws are recommended for higher-performance systems but were not required here.

**Placeholders**

* *\[Diagrams showing weld locations (structural only).]*
* *\[O-ring groove relative to chamber ID.]*
* *\[Step-by-step viewport assembly photos.]*
* *\[Details of salvaged KF-to-bolt-flange adapter (Aryamman).]*

#### Magnetron

Design closely follows CMU’s published documentation (**link TBD**).

**Material choice**

* Mild steel is magnetic (required) but rusts → outgassing risk.
* Stainless is non-magnetic.
* Solution used: mild steel plate with **electroless nickel plating**. Sand off existing rust, plate immediately before fresh rust forms.\
  Do **not** use powder coating or galvanizing — they are not vacuum-compatible.

**Placeholders**

* *\[Actual CMU hyperlink.]*
* *\[Photos of the finished magnetron.]*
* *\[Full source list / citations for the geometry.]*
* *\[Cooling details if water cooling is used.]*

#### Gas Flow System

1. **Estimate required flow**\
   Based on chamber volume, turbo speed, and target pressure.\
   Strike at \~0.1 mbar, then reduce to 0.01–0.001 mbar for sputtering. Pressure is a dynamic balance between continuous turbo pumping and continuous argon inflow.
2. **Select MFC**\
   Second-hand units are cost-effective. Each MFC is calibrated for a specific gas. Use manufacturer gas conversion factors (GCF) to operate with argon if the unit was calibrated for another gas (e.g. N₂ or O₂). Typical GCF for Ar relative to N₂ is ≈ 1.39–1.40. Accuracy is reduced (±5 % typical) when using conversion factors.
3. **Argon supply**\
   Cylinder + regulator. Choose tubing (metal or plastic) compatible with the regulator outlet. MFCs almost always use VCR fittings → NPT-to-VCR or push-fit-to-VCR converters are commonly required. VCR gaskets are single-use (plastic deformation).
4. **MFC to chamber**\
   VCR → KF adapter + KF size reducer if needed. Always verify male/female gender at every joint.

**Placeholders**

* *\[Block diagram of entire gas path with fitting call-outs.]*
* *\[Links to MFC, argon, fittings, Fifer textbook, and GCF explanation.]*
* *\[Swagelok reference videos.]*

***

### Standard Operating Procedure (SOP)

**Assigned to Aryan in the original notes.**

**Placeholder — Full SOP**\
*\[Aryan to write the complete step-by-step operating procedure covering: system checks, pump-down sequence, gas introduction, plasma ignition, deposition, shutdown, and emergency stops. Include exact pressure set-points, voltage ramp recommendations, and gauge switching sequence once the Penning interlock threshold is known.]*

***

### Startup / Shutdown Checklists

These checklists are derived from the safety notes and are intended to be printed and kept next to the machine.

#### Safe Startup Sequence (high-level)

1. Visual inspection: no obvious damage, all cables secure, chamber clean and empty of tools.
2. Verify all valves in correct initial state.
3. Start rotary vane pump.
4. When Pirani indicates sufficiently low pressure, start turbo pump.
5. Wait for base pressure (Penning may be turned on only after its interlock threshold is reached).
6. Introduce argon via MFC and stabilize at strike pressure.
7. Apply high voltage (slowly ramp with variac) and ignite plasma.
8. Adjust argon flow / voltage to reach desired sputtering pressure and rate.
9. Begin deposition timer / substrate exposure.

#### Safe Shutdown Sequence (high-level)

1. Reduce / remove high voltage.
2. Stop argon flow.
3. Allow system to pump for a short time.
4. Turn off Penning gauge (if on).
5. Turn off turbo pump (follow manufacturer cool-down / spin-down procedure).
6. When turbo is safe, vent the chamber **only** after turbo and Penning are off.
7. Turn off rotary pump.
8. Isolate power and gas supplies.

**Placeholder**\
*\[Expand into detailed, numbered checklists with exact pressure numbers, switch locations, and interlock status once the system is fully characterized.]*

***

### Automation

**Placeholder**\
*\[Describe any existing or planned automation: pressure interlocks, MFC set-point control, high-voltage interlock, data logging, etc.]*

***

### Software

**Assigned to Aryan in the original notes.**

**Placeholder**\
*\[Aryan to document any control software, scripts, GUI, data-logging tools, or Arduino/PLC code used.]*

***

### Improvements

**Placeholder**\
*\[List of planned or desirable upgrades: better load-lock, water-cooled magnetron, RF capability, thickness monitor, improved interlocks, etc.]*

***

### Troubleshooting & Failure Modes

| Symptom                                  | Possible Cause                                                 | Action                                                                                      |
| ---------------------------------------- | -------------------------------------------------------------- | ------------------------------------------------------------------------------------------- |
| Cannot reach base pressure               | Leak (most common), outgassing material, pump issue            | Leak-check with helium or sequential isolation; bake if possible; check O-rings and gaskets |
| Slow pump-down                           | Large virtual leak, dirty chamber, water vapor                 | Thorough cleaning, longer pump, mild bake                                                   |
| Penning gauge arcs / fails               | Powered on at too high pressure                                | Replace head if damaged; enforce strict Pirani interlock                                    |
| Plasma will not strike                   | Pressure too high/low, voltage too low, gas not flowing, short | Check gauges, MFC, variac setting, wiring                                                   |
| Unstable plasma / arcing                 | Contaminated target, poor grounding, water vapor               | Clean target, verify ground, improve base pressure                                          |
| High voltage shock / unexpected behavior | Poor grounding, capacitor not discharged                       | Immediate power-off, re-verify grounding and discharge procedures                           |

**Placeholder**\
*\[Expand with photos of common failure signatures and more detailed diagnostic trees.]*

***

### Glossary

| Term          | Meaning                                                          |
| ------------- | ---------------------------------------------------------------- |
| KF / NW       | Klein Flange / Quick Flange — clamp-style vacuum flange          |
| ISO-K / ISO-F | ISO clamp / bolted flanges                                       |
| CF            | ConFlat — knife-edge metal-seal flange                           |
| VCR           | Vacuum Coupling Radiation — high-integrity metal-gasket fitting  |
| NPT           | National Pipe Thread                                             |
| MFC           | Mass Flow Controller                                             |
| sccm          | Standard cubic centimeters per minute                            |
| Pirani        | Thermal-conductivity vacuum gauge (rough to medium vacuum)       |
| Penning       | Cold-cathode ionization gauge (high vacuum)                      |
| Variac        | Variable autotransformer                                         |
| PEEK          | Polyether ether ketone — high-performance non-conductive polymer |
| GCF           | Gas Conversion Factor (for MFCs)                                 |

***

### India-Specific Sourcing Notes

Several components proved difficult or impossible to source locally and required import or custom machining:

* NPT-to-VCR converters
* Certain KF-to-bolt-flange adapters (salvaged from surplus valves; one candidate found in the US)
* Specific MFC models and VCR gaskets
* High-quality Viton O-rings of exact sizes in some cases

**Workarounds used**

* Local appliance repair shops for microwave transformers and diodes.
* Custom machining of adapters.
* Second-hand MFCs via international marketplaces.
* Electroless nickel plating performed locally after careful rust removal.

**Placeholder**\
*\[Expand into a full table of “hard-to-source” items with exact workarounds, vendor contacts (if shareable), and lead times.]*

***

### To-Do / Missing Content

(Retained and organized from original notes)

#### Power Supply

* [ ] Link all related videos
* [ ] Re-check capacitor-discharge wording
* [ ] Photo / link for HV gloves
* [ ] Proper circuit diagram
* [ ] Photos of each subsection + original open setup (including any relevant incident)

#### Vacuum System

* [ ] Turbo-to-chamber geometry diagram
* [ ] Expand on load-lock alternative
* [ ] Verify exhaust-line wording (Aryamman)
* [ ] Verify Viton-on-CF description
* [ ] Photos of KF assembly, O-rings, flange sizes
* [ ] Exact Penning interlock pressure

#### Chamber

* [ ] Weld-location diagrams
* [ ] O-ring groove diagram
* [ ] Viewport assembly photos & steps
* [ ] Salvaged adapter details (Aryamman)
* [ ] Exact part name of US-found adapter

#### Magnetron

* [ ] CMU documentation hyperlink
* [ ] Photos of this build’s magnetron
* [ ] Full source citations

#### Gas Flow

* [ ] Component links
* [ ] Fifer textbook link / confirmation
* [ ] GCF calculation source
* [ ] Full gas-path block diagram with fitting call-outs
* [ ] Swagelok references

#### Other

* [ ] Complete BOM with costs and links
* [ ] Populate Resources with live links
* [ ] SOP (Aryan)
* [ ] Software (Aryan)
* [ ] Automation section
* [ ] Improvements section
* [ ] All photos currently marked TBD


# tube-furnace

This is the official HackerFab IITB documentation for the tube furnace.

## The Tube Furnace

A tube furnace is a special piece of equipment widely used in many labarotaries to carry out various chemical reactions in a controlled manner. In the case of semiconductors, tube furnaces are used mainly for carrying out the oxidation of Silicon or any type of diffusion doping.

$$
\Large \mathrm{Si} + \mathrm{O\_2} \xrightarrow{1100°\mathrm{C}} \mathrm{SiO\_2}
$$

The tube furnace we have built at HackerFab IITB can currently perform oxidation, but can be modified to carry out any high temperature process. This is what it looks like!

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FOB9dF9bWZiGogsnh3GZF%2F84B24CF3-BC6E-421A-8579-179F10D9CB89_1_102_a.jpeg?alt=media&amp;token=f761b009-189a-4181-bef4-eee46476500a" alt=""><figcaption></figcaption></figure>

## Specs

Standard Operating Temperature : 1100±5°C

Heating Zones : Single Zone Configuration

Tube Dimensions : 60mm OD, 800mm Length

Tube Material : Quartz

Temperature Controller : Multispan UTC-4202G+

## Disclaimer

This documentation is provided for educational and informational purposes only. Building and operating a tube furnace involves extreme temperatures, high electrical currents, and hazardous materials. By following this guide, you acknowledge that you are doing so at your own risk. The authors and HackerFab IITB are not responsible for any property damage, injury, or loss of life that may occur as a result of attempting this project. Always consult a qualified professional if you are unsure about electrical wiring or high-temperature systems. An entire paragraph on safety is given below.

## Bill of Materials

Links to all the materials will be provided in another table separately.&#x20;

<table><thead><tr><th width="153.6640625">Material</th><th>Purpose</th><th>Quantity</th><th>Cost</th><th width="149">Net Cost (INR)</th></tr></thead><tbody><tr><td>Quartz Tube (67mm dia, 800mm)</td><td>Tube</td><td>1</td><td>Vendor will give a Quotation</td><td>2500</td></tr><tr><td>Kanthal A1 14 SWG</td><td>Heating Element</td><td>1 kg</td><td>Depends on vendor (INR 3-5k)</td><td>4703.39</td></tr><tr><td>Kanthal A1 20 SWG</td><td>A "brace" for the heating element</td><td>100 g</td><td>Depends on the vendor</td><td>300</td></tr><tr><td>Whytheat A</td><td>Refractory Cement</td><td>25 kg</td><td>INR 168/kg. The rate for Whytheat is pretty standard</td><td>4200</td></tr><tr><td>Inner PVC Pipe (75mm dia, 1m length) with the cap</td><td>To create the cement mold</td><td>1</td><td>Depends on vendor, but PVC pipes are in every hardware store and they are pretty cheap.</td><td>300</td></tr><tr><td>Outer PVC Pipe (160 mm dia, 1m length) with the cap</td><td>To create cement mold</td><td>1</td><td>Depends on vendor</td><td>500</td></tr><tr><td>Steel Rod of diameter 7mm and length 60 cm</td><td>Used to coil the kanthal</td><td>1</td><td>Depends on the steel shop. They will probably just cut a bigger rod</td><td>100</td></tr><tr><td>Ceramic Wool of density 96g/cc</td><td>Used as insulation around the refractory cement cast</td><td>10 kgs</td><td>110/kg, again the rate for ceramic wool is pretty standard.</td><td>1100</td></tr><tr><td>MS Sheets (3 by 4 feet)</td><td>Will be made into the enclosure</td><td>4 sheets (~30 kgs)</td><td>Go into the steel market and buy it yourself. The cheapest rate I found it at in Mumbai was 90/kg. There were some vendors trying to sell it to me at 200/kg as well.</td><td>2700</td></tr><tr><td>Steel angles (100cm)</td><td>To provide mechanical support and strengthen the steel enclosure</td><td>2</td><td>Again, depends on the vendor. They are pretty cheap and you should be able to get them under 200 rupees.</td><td>400</td></tr><tr><td>Screws</td><td>To make one face of the steel enclosure removable</td><td>20</td><td>1 rupee per screw</td><td>20</td></tr><tr><td>Temperature Controller (Multispan UTC-4202G+)</td><td>For PID Temperature control</td><td>1</td><td>Buy the temperature controller as per budget. Read the section on the temperature controller to get to know more</td><td>3300</td></tr><tr><td>Solid State Relay (SSR) 40 Amps</td><td>For electrical isolation, and helps the temperature controller do its job using PWM</td><td>1</td><td>As per MRP. This will be available in any electronics store</td><td>250</td></tr><tr><td>Aluminium Heat Sink</td><td>To help regulate the temperature of the SSR</td><td>1</td><td>As per MRP. This may take some time to find.</td><td>200</td></tr><tr><td>Thermal Paste</td><td>Goes between the heat sink and the SSR</td><td>1</td><td>As per MRP. You'll find this in any laptop repair shop</td><td>100</td></tr><tr><td>Bakelite Connector 30 Amps (6-Way open connection)</td><td>Connects Mains voltage, SSR and heating element. This is where all the electronic components meet.</td><td>1</td><td>As per MRP. This may take some time to find.</td><td>30</td></tr><tr><td>Mains Switch (Single Pole MCB, 25 Amps)</td><td>Turn this on to let power from your outlet into your circuit</td><td>1</td><td>As per MRP. You'll find this in your normal electronics store</td><td>300</td></tr><tr><td>Heating Switch (Single Pole MCB, 2 Amps Rocker type)</td><td>Turn this on to let power from your circuit into your heating element</td><td>1</td><td>As per MRP.</td><td>300</td></tr><tr><td>LED Light (Big one)</td><td>Indicates whether the tube furnace is on or off</td><td>2</td><td>As per MRP.</td><td>40</td></tr><tr><td>K type MI thermocouple (Mineral insulated)</td><td>To measure the temperature. The thermocouple should be of appropriate dimensions and should be mineral insulated</td><td>1</td><td>Vendor will give you a quotation</td><td>1950</td></tr><tr><td>Internal wiring (2.5 sqmm)</td><td>To connect the high current parts of the circuit</td><td>1m</td><td>35-50/meter</td><td>50</td></tr><tr><td>Internal wiring (1 sqmm)</td><td>Normal electrical wires to connect everything</td><td>2m</td><td>20-30/meter</td><td>60</td></tr><tr><td>Metal Box</td><td>To keep all the electrical components</td><td>1</td><td>You can find some scrap box or make this yourself</td><td>0</td></tr><tr><td>Quartz Boat with hook</td><td>To keep the silicon wafer</td><td>1</td><td>Vendor will give a quotation</td><td>100</td></tr><tr><td>Push-Pull Quartz rod (Length 1m)</td><td>To push and pull the quartz boat in and out of the tube furnace</td><td>1</td><td>Vendor will give a quotation</td><td>600</td></tr><tr><td>Standard Ammeter</td><td>To measure the current going in the coil</td><td>1</td><td>Buy the standard one you see in labs</td><td>500</td></tr><tr><td>Standard Voltmeter</td><td>To measure voltage across mains</td><td>1</td><td>Buy the standard on you see in labs</td><td>500</td></tr><tr><td>Porcelain connector (15 Amps)</td><td>For connecting the coil to standard wiring</td><td>2</td><td>20/piece</td><td>40</td></tr><tr><td>Ceramic beads</td><td>To safely insulate the exposed coil</td><td>1 kg</td><td>You will need much less than 1kg. We found some in our lab, so we didn't have to buy any.</td><td>150</td></tr><tr><td>Build Cost</td><td>Net build cost, if you don't mess anything up</td><td>-</td><td>-</td><td><strong>31,543.39</strong></td></tr><tr><td>Angle Grinder</td><td>To cut steel, kanthal, a very useful tool to have in general</td><td>1</td><td>You might get this below 2500</td><td>2500</td></tr><tr><td>Cutting Wheel</td><td>The angle grinder will be fitted with this, buy an extra incase the first one wears off</td><td>2</td><td>50/piece</td><td>100</td></tr><tr><td>Drill</td><td>Will be used for tapping the steel plate</td><td>1</td><td>Again, you might get this cheaper</td><td>3000</td></tr><tr><td>Thread Bit</td><td>For the drill</td><td>1</td><td>Again, you might get this cheaper</td><td>150</td></tr><tr><td>Aluminium Paint</td><td>So that the steel enclosure does not rust</td><td>1</td><td>350</td><td>350</td></tr><tr><td>Turpentine Oil</td><td>You will most likely need it to remove any paint off of your skin</td><td>1L</td><td>150</td><td>150</td></tr><tr><td>Multimeter</td><td>You should have this by now</td><td>1</td><td>200</td><td>200</td></tr><tr><td>Clampmeter</td><td>Not necessary, but useful</td><td>1</td><td>300</td><td>300</td></tr><tr><td>Fabrication Cost</td><td>To fabricate the coil and the steel enclosure you will need access to a lathe and a welding machine.</td><td>-</td><td>This cost is variable, and depends on how much your vendor charges you.</td><td>3447</td></tr><tr><td>Net Budget</td><td>-</td><td>-</td><td>-</td><td><strong>35,500</strong></td></tr></tbody></table>

## The Build

### The Furnace

This build covers the conversion of the Kanthal wire into a coil, creating the refractory cement cast, covering it with ceramic wool and fabricating the steel enclosure. Quite a bit of this is laborious work, so you might need a few keen helpers here and there, be ready to ask for help! After all of this, the furnace should look like this :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FuVdeZbb7fVh8t4xT3cLo%2FE16B28F8-F306-4B6A-ABBD-8C4B7FE10522_1_105_c.jpeg?alt=media&amp;token=5c033f46-c036-4484-a0f8-79e51ad6145d" alt=""><figcaption></figcaption></figure>

#### The Heating Element

First off, you need to buy approximately 1 kg of Kanthal A1 (14 Gauge). It should look a bit like this :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FXtuVpf3NXlfv4iorXQ8e%2FD36988C8-48BC-4FC9-A0F5-99B9BDEBC26C_1_201_a.heic?alt=media&amp;token=20ac2f4d-731f-4418-ba8e-61cff2b03a49" alt=""><figcaption></figcaption></figure>

Some basic questions you might have:

* Why Kanthal A1?
* Why 14 Gauge Kanthal?
* How did we decide how much Kanthal to buy?

All these are genuine questions, and I will discuss them after I show you how to fabricate the coil.

#### 1. Fabricating The Coil

To fabricate the coil:

* Use a lathe operated by an experienced professional.
* Provide the operator with a 8 mm diameter steel rod (which serves as a mandrel).
* Wind the Kanthal A1 wire around the 8 mm mandrel.
* **ENSURE that you leave at least 1 meter of loose Kanthal wire on each end!**
* Maintain a 3.5 mm pitch between each turn.
* Measure the finished coil's resistance with a multimeter.
* Confirm that the coil is longer than 5 m.

After the coil has been machined, it should look like this (notice the loose wire at the ends) :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fett70qYW7fYgMAMx7PWg%2FEC823C91-2E64-4783-84AE-D3A197F41508_1_105_c.jpeg?alt=media&amp;token=6555e750-9320-4878-9be4-881b7a0744a1" alt=""><figcaption></figcaption></figure>

#### If you want to design the coil specifications by yourself

This is something totally optional, which you can do if you are adventurous in nature. For others, just skip this block and go to "2. Making The Cement Cast".

The first thing you need to keep in mind, that the net resistance of the coil

To the future Rushat : pls fill this after the furnace fabrication is done

#### 2. Making The Cement Cast

Before starting this, ensure you have the following things :

* Kanthal A1 Coil of minimum length 5m (if you are following our design)
  * Note : Do not worry if the coil is not 5 meters long, just read this section to get a feel for what we will be doing, and then read section 2.2.
* Inner and outer PVC pipes with their caps
* Whytheat A or K Refractory Cement (25 Kgs)
* A minimum of 4 people to help you

#### 2.1 The Coiled Coil

The precise shape of our heating element would be a coiled coil as shown below:

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FKjeTYu84UjivrDZeLnm7%2FScreenshot%202026-07-28%20at%208.36.15%E2%80%AFPM.png?alt=media&amp;token=0abe133e-26e8-449f-bbb8-e8c1ac3b554f" alt=""><figcaption></figcaption></figure>

The image is a bit poor, but this is a model of the actual heating element inside the furnace.&#x20;

Here is a general workflow of what we will be doing next :

1. Coiling the coil around the inner PVC (2.1)
2. Using this to create a PVC mould (2.2)
3. Pouring in the cement, and letting it sit (2.3)
4. Curing the cement (2.4)

Firstly, when we pour the cement, none of it should go into the inner PVC, so you must install the caps onto it before coiling the coil onto it. Then make even markings at a distance of 3cm, leaving more than 10 cm of space on each side. Like this :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2F9RYvgMWGJtA0SpRf2pjJ%2F3E2AB81C-FB06-4460-8467-59E7384A50BA_1_102_o.jpeg?alt=media&amp;token=e9b0ada0-41fb-4044-bd72-1392ad4bbeea" alt=""><figcaption></figcaption></figure>

Now, the hard part. At one end - tie the Kanthal coil's loose end with a Kanthal wire of lesser gauge. Make maximum use of force and tie it as hard as humanly possible. Make sure you have more people to help you. Notice the place it which you tie it must be that place where the loose end starts and the coil ends :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2F3wzVM6wiRJiIED64ZquY%2FCD83909E-DFD4-4CFE-8F5C-0AA93E75C447_1_102_a.jpeg?alt=media&amp;token=946fdb3a-b547-4afa-b9c2-24f4385c3390" alt=""><figcaption></figcaption></figure>

Make sure you let the loose end be as long as possible on both sides, since this is where the heating element will be connected to the circuit. They essentially serve as the terminals of the heating element!

Now, you'll need help for this as well - actually coiling the coil around the PVC. Again, make sure it is as tight as humanly possible, and while keeping this tightness - you must tie the other end of the coil with Kanthal of a lesser gauge :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FvkGEb7o4bGFoYrCZ4Zw5%2FCA61A4A5-4567-41F2-942A-4CE2C74A80FD_1_105_c.jpeg?alt=media&amp;token=9905d3bc-ce90-43de-aac6-e93e05b16c3e" alt=""><figcaption></figcaption></figure>

After you have toiled this much, enjoy the fruits of your labour by measuring the coils net resistance, since this will decide how much current will pass through and how hot it will theoretically get!

Thats it! The coiled coil is done!

#### 2.2 The PVC Mould

The PVC mould, at the end of the day, is a mould. The only purpose it serves is to shape the cement cast. However, there are some things you must take into consideration before pouring in the cement :&#x20;

1. Make holes to let the loose Kanthal ends out
2. Install the PVC pipe caps in such a way so that water can be drained from the cement

Number 1 is easy, just measure where you want your Kanthal to poke out and drill a hole there.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FDiR6hZ3H6tI1BVBpzSPe%2F6E94851C-1CFE-4B20-B668-5D62D707C14C_1_105_c.jpeg?alt=media&amp;token=6c1e2077-c690-4a7c-a6f4-515ae56e4a7f" alt=""><figcaption></figcaption></figure>

Number 2 is a bit tricky, and requires modifying with the PVC pipe caps a little. Drill a hole the diameter of the inner pipe (75 mm) in the outer PVC's cap. You will need a lathe for this :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2F44YdW1ZzbXFG3hhAGCtV%2FScreenshot%202026-08-03%20at%208.13.01%E2%80%AFPM.png?alt=media&amp;token=15b20e94-0449-434f-83ce-36299cab8552" alt=""><figcaption></figcaption></figure>

Once that is done, just put the cap onto the outer PVC and cover the inner parts of the cap with thermocol like so :

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2F92sTo5LQy76x6mT35wG3%2F06B235EE-E54D-45F2-8C22-DB4F00D382A4_1_105_c.jpeg?alt=media&amp;token=faf5c5e9-39ad-4edf-b46f-21d2c5970798" alt=""><figcaption></figcaption></figure>

This leaves an essential gap between the PVC cap and the cement, so that they don't stick and the water can drain through it. Now, carefully lower the coiled coil on the inner PVC and fit it into the hole on the outer PVC cap. Make sure the coil maintains a uniform pitch throughout this procedure.

![](https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fjx99Cwxveen2JDcJEVYq%2F56A03145-37BB-49F9-92B6-9999C89FF784_1_105_c.jpeg?alt=media\&token=2704e0c3-fe42-44ad-b05d-00c937086677)&#x20;

Now that this is done, only install the inner PVC cap on one side, which is the side from which we will pour the cement. It should not be installed on the other side so that water can drain out.&#x20;

#### 2.3 The Cement Pour

This is the last and final step after which you will have a ready to use heating element.&#x20;

* Mix the cement with water in a 4:1 ratio (4 parts water 1 part cement)
* Pour it inside the mould
* Let the mould sit for 3-4 days
* Water it everyday (Pour water on it)

The mould:

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fr8U7i0ocNGNHRN62gXUT%2F33B681BD-9E69-49A0-A821-009E47148EE6_1_105_c.jpeg?alt=media&amp;token=328ee5b9-7a71-4fee-b757-4bd117f84cbe" alt=""><figcaption></figcaption></figure>

After pouring, it should be kept upright and secured:

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FLyhT4e093H8wXvu6Zr1w%2F2AFDBF07-8FA3-4591-B392-2ED3FF64D3DC_1_105_c.jpeg?alt=media&amp;token=32818620-16c6-4136-be13-4eb77540d417" alt=""><figcaption></figcaption></figure>

Some itty bitty things you need to worry about :&#x20;

* There should be no bubbles in the cement&#x20;
  * To remove all the bubbles, take a steel rod and "churn" the cement
  * MAKE SURE to not disturb or touch the coil while doing this
* The coil should not move because of the cement, to ensure this you need to coil the coil around the inner PVC as tightly as possible.

#### 2.4 Curing the Cement

Removing the PVC pipes utilizes quite a bit of firepower. Firstly, cut of the outer PVC using an angle grinder :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FXBnUl8ZooqVMhVLSdafG%2F51D6C351-45E1-4C61-BF92-688577C5871D_1_105_c.jpeg?alt=media&amp;token=6b8116c2-d4d9-438b-b97a-5b44be0bf58b" alt=""><figcaption></figcaption></figure>

The uncured cement should look something like this, even after trying our hardest to remove all the bubbles, some were still there :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FYJLckLsKwDwIPKRtTPbs%2F9756E15E-6BC1-4BBF-B984-BD95D91117A1_1_105_c.jpeg?alt=media&amp;token=563eb813-1fd3-4a99-ae89-e2ccdf4dd3cf" alt=""><figcaption></figcaption></figure>

There is no peaceful way to remove the inner PVC. Use a oxygen blowtorch to melt the inner PVC off the cement :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FZ84bogWCExpVrQJbkUYr%2F94E06CCD-A69D-4686-A7DA-D65C7963D83A_1_105_c.jpeg?alt=media&amp;token=7628c4e6-f336-423d-a7d0-d08c55634ef3" alt=""><figcaption></figcaption></figure>

Then, to the extruding Kanthal Coil ends, twirl Kanthal of a lesser gauge around them to make them thicker and being able to take more current. (You can see this in the next picture)

#### 2.4.1 The Wait

It'll take 3-4 days for the cement to dry completely. In the meantime, you need to complete the electrical circuit, the directions for which are given after the furnace build.

#### 2.4.2 Curing the Cement

After the cement has been completely dried, you will need to cure it. You should have the circuit ready by the time the cement has dried, since it takes around 3-4 days to dry, and the circuit can be made within 2 days (1 day to buy everything, 1 day to build it).

#### MAINTAIN UTMOST SAFETY AND PRECAUTION WHILE DOING THIS!!

Cover the loose ends of the Kanthal wire with ceramic beads, and connect them to live and neutral using porcelain connectors. Before switching the mains switch on, make sure everything has been securely connected. Set the temperature controller to K-type and set to 100 degrees celsius.

Switch the mains supply on, and let the cement cure for half a day. Do not let anyone go near the heating element. Any contact with it will kill you instantly.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fi6Lflkz0yCzziLNDF01g%2FBAE13695-5342-4AEE-819C-73C126151927_1_105_c.jpeg?alt=media&amp;token=4446b23d-aaea-472d-8447-c26fe9bdbcc0" alt=""><figcaption></figcaption></figure>

#### 2.5 Steel Box Fabrication

Firstly, cut your steel sheets into appropriate dimensions, and then weld them together to create a steel envelope of sorts.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FbOvMgJbjqAR2v0z7O6tF%2F6A0D6A5B-2326-4DA9-A6CB-E83872783B18_1_102_a.jpeg?alt=media&amp;token=d042acd6-74de-4b51-a520-18125ede3fe6" alt=""><figcaption></figcaption></figure>

Using the angles, cut them to the appropriate dimensions and insert them into this frame to help with rigidity and get rid of that depression you see on the top plate. Drill holes in appropriate places since we will be screwing in the front plate.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fgqkx60UBfaDuE9OJLMJH%2F3FE37E71-A9E2-4113-B4F9-764680E86359_1_102_a.jpeg?alt=media&amp;token=8f514959-ba9c-4e85-84a5-c194e062c21d" alt=""><figcaption></figcaption></figure>

We needed help with welding, since we are not trained to weld. In this image you can see how we installed the angles and welded them with appropriate slots for screws.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FXVGnloa4djc8BVlxMVUp%2FCB2D16C0-3AA8-4E3E-A42D-87503CA54361_1_102_o.jpeg?alt=media&amp;token=c534153a-8b52-4c55-9d61-6b524521fcb6" alt=""><figcaption></figcaption></figure>

Make a square hole in the bottom plate and weld it in, make sure to leave the top plate uninstalled:&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FBJxC9ivz9qDJea329vIn%2F3368D49D-40FC-47FD-B626-0BE0391579F5_1_102_a.jpeg?alt=media&amp;token=caf52bc5-b4fa-4973-9852-606b2cfdbc73" alt=""><figcaption></figcaption></figure>

#### 2.6 Insulation

This is certainly the most itchy part of the entire thing. Ceramic wool is dangerous to your lungs and can cause chronic diseases. Please wear a mask and thick gloves to protect yourself from the wool. This is me lifting up the entire roll of ceramic wool. I regret not wearing a full sleeve tshirt, so I highly recommend wearing one - unless you want your hands to itch unbearably.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FJiTSv1V740SihyCHFS4a%2F2ED1152C-B197-43F9-AA8A-2B7E39D5B82D_1_105_c.jpeg?alt=media&amp;token=dc18a44d-fe14-417c-9f44-f25bcd0b01a4" alt=""><figcaption></figcaption></figure>

Do some jugaad to find out the perfect cutout for the top plate :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FhTd4TiWpfRlnAZ3D4VTp%2F56B2B3AB-8A3A-4413-B2F1-EA490956CDB2_1_106_c.jpeg?alt=media&amp;token=688ee521-c20b-4af2-a426-314870ada985" alt=""><figcaption></figcaption></figure>

And then after cutting it with a knife, fit it on the bottom plate :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FvYrTmPA50fRUCOLWxGkS%2FCF0CCEA6-CDB5-4CB6-8233-884D0443C3CC_1_105_c.jpeg?alt=media&amp;token=6f52b16b-8e84-4f40-8260-6863b07e75de" alt=""><figcaption></figcaption></figure>

The next step is quite a bit of manual labor, and it involves wrapping the cement cast in as much insulation as you have available. Get one person to do the rolling, one person to slide the wool beneath the role, and one person to cut off the excess roll, after all this you'll get a very well packed roll of insulation :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FLVemxtrl0qafgavPr3Mw%2FA69507C0-CE1E-40AA-8423-70F8E8FEB9E9_1_105_c.jpeg?alt=media&amp;token=8e6730cf-6f1b-4048-be42-b442be867b22" alt=""><figcaption></figcaption></figure>

Now, just pack the gaps with whatever ceramic wool you have left, screw in the top plate and you're good to go!&#x20;

Cover the loose ends of the Kanthal with ceramic beads, and using a porcelain connector connect it to live and neutral. Stuff some ceramic wool around the inner cement and insert the quartz tube into it so that it does not touch the cement and is centered. Paint the steel enclosure with aluminum paint and connect it to ground. Voila! The tube furnace is ready! This was our tube furnace just after it was built :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FqPa8wDvvojBXS2tLRNlx%2F60875E49-C4B3-431C-A5C4-9B5A587117D8_1_105_c.jpeg?alt=media&amp;token=c6c3406e-b989-47e0-a484-690a9fc55e7c" alt=""><figcaption></figcaption></figure>

After moving it to our lab, and spray painting the circuit box with black spray paint from Mr. DIY :&#x20;

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FC3tiZIYmW2O91sOGaNnV%2F9D57DB4E-E240-4D69-8EA1-18B3E310B406_1_102_a.jpeg?alt=media&amp;token=96a46e76-cce7-436c-b598-dd397b5ecd2a" alt=""><figcaption></figcaption></figure>

For any questions regarding the build, please email me at <rushat.dixit@gmail.com>, or join our discord server : <https://discord.gg/EcQqY8Dmv3>

The SOP has been included separately. &#x20;

### The Circuit

#### Component List

* Multispan UTC-4202G+ PID Controller
* Fotek SSR-40DA (40A)
* Bakelite Connector (30A)
* K-Type Minerally Insulated Thermocouple
* Digital AC Voltmeter
* Digital AC Ammeter
* Heating Switch(MCB 25A)
* Main Switch

Here are the datasheets for the Temperature Controller and SSR

{% file src="/files/qNzJYZ1CwVyXvFenPcTf" %}

{% file src="/files/TRYWNj4yPTzLxqacBbjF" %}

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fcyw9t0UkCyA6hIHIbyTy%2Fimage.png?alt=media&amp;token=502f63ca-67e8-45bb-9b65-9d6851edc1df" alt=""><figcaption></figcaption></figure>

Here is the pinout of the temperature controller,the connections we've made are:

1. Pin 1 - Live wire
2. Pin 2 - Neutral wire
3. Pin 6 - SSR Pin 4 (DC-)
4. Pin 7 - SSR Pin 3 (DC+)
5. Pin 8 - K-Type Thermocouple(yellow wire)
6. Pin 9 - K-Type Thermocouple(red wire)

We used K-Type Thermocouple where the positive wire was yellow and the negative wire was red.

Note: You can also make your own controller we just decided to use the one we already had in the lab.

Here's a colour coding chart depending on what type of thermocouple you use

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FbbnJ0Hnw1EVQgNawZgpK%2Fimage.png?alt=media&amp;token=6b088be3-4257-437f-abf5-c15f1c5a1130" alt=""><figcaption></figcaption></figure>

Here is the SSR connection diagram

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FMvnzf3RsI4psi8ysrurb%2Fimage.png?alt=media&amp;token=da28057f-77fb-4529-981c-93cca06112d7" alt=""><figcaption></figcaption></figure>

As mentioned above we've connected pin 3 of the ssr to pin 7 of the controller and pin 4 to pin 8

Note: I've attached the datasheet and connections for the fotek 40DA ssr, but we've used the sibass one but the functionality remains the same

Bakelite Connector: We've used it to interface all the connections we need safely. It is rated for 30A

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FCureyD1MSTT2YK6zOt5o%2Fimage.png?alt=media&amp;token=8001a87b-ee48-4eb2-aef1-a24d58a50458" alt=""><figcaption></figcaption></figure>

This is what the overall circuit looks like:

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FKRppmG9WB0tv045nZNAR%2Fimage.png?alt=media&amp;token=e5cb57fe-e17b-4a37-b529-460e9e9a672e" alt=""><figcaption></figcaption></figure>

## Safety

As students, we tend to disregard the matter of safety under the impression "kya hi ho jaayega?". However, the tube furnace, or as a matter of fact any project you pursue, should always be carried out following the appropriate safety protocols. This is a project, wherein ignoring safety protocols may result in heavy injury or the loss of life. We at HackerFab IITB always follow the due protocol, and encourage you to do so as well.

### Electrical Safety

The furnace runs on mains power and draws significant current (10-12 Amps). A simple mistake like touching the heating element can be fatal. Take significant precaution, I have listed a few golden rules:

#### 1. Always ground any metal enclosures

The furnace enclosure is made of MS (mild steel) and can carry any leaking current. The entire enclosure must be securely grounded. Always check whether all metal bodies are grounded with a multimeter (by checking continuity) before starting the furnace.

#### 2. Isolate Power

Put all the electronic components inside a metal box. This metal box should never be opened while the furnace is running. Do not touch any of the wiring, or the electronics inside the box while the furnace is plugged in. Always unplug the system before maintenance.

#### 3. Wire Gauges

Ensure you strictly follow the BOM for wiring. Use the 2.5 sqmm wire for the high-current AC lines and heating element connections to prevent wire melting and electrical fires.

### Thermal Safety

Operating at 1100°C means standard safety gear is not enough. You will get burnt even if you touch a thousand degree quartz boat with specialised gloves.

#### 1. Fire Hazard

Keep the furnace on a non-combustible surface (like a concrete table, thick ceramic tiles or a steel table). Ensure there are no flammable materials, chemicals, or papers within at least a 1-meter radius. Always keep a fire extinguisher nearby.

#### 2. Never leave unattended

Do not leave the furnace unattended while it is ramping up or holding at high temperatures.

#### 3. Cooling Time

The furnace will remain dangerously hot for hours after the power is turned off. Do not attempt to touch the outer enclosure, and never open the tube or remove the quartz boat until the internal temperature has dropped below 100°C.

#### 4. Quartz never looks hot

Quartz, even above a thousand degrees celsius, will always look transparent and never turn red. Let the quartz boat cool after removing it.

### Material Handling Hazards

Always check the MSDS of the material in question before doing anything with it. You could play with a harmless looking material, and it could turn out to be a carcinogen (ceramic wool)!

#### 1. Ceramic Wool

Ceramic wool fibers can cause severe respiratory irritation and long-term lung damage if inhaled. Always wear a high-quality N95 or P100 respirator mask, safety goggles, and gloves when cutting, packing, or handling the ceramic wool.

Here is the MSDS, I urge you to take a look at it:

{% file src="/files/XCzYsTAa6ReYyt8pYsXJ" %}

#### 2. Quartz Glass

The quartz tube and boat are highly susceptible to thermal shock. Pulling the boat out too quickly while it is hot will cause it to shatter. Handle quartz with care to avoid cuts.

This is certainly not as bad as ceramic wool, but you should still check the MSDS out:

{% file src="/files/JO4h17RLGYGNfs8mBjUB" %}

#### 3. First Burn-In

The first time you fire up the furnace, the Whytheat refractory cement and some components will off-gas moisture and potentially toxic fumes. The first run must be done in a highly ventilated area or under an exhaust hood. This point may feel unlikely, but trust me, the cement will fume out the first time after being cured.

Again, not as bad as the ceramic wool. Here is the MSDS:

{% file src="/files/BRHdpve3ko2Ew4q2XF24" %}


# dopant (diy)

DIY:

Ingredients

* TEOS (Tetraethyl orthosilicate)
* Water
* Catalyst
* Alcohol solvent (Ethanol or Isopropyl Alcohol)
* Dopant atoms

The Chemical Mechanism When TEOS and water react, they form a spin-on glass (SOG). Because these two chemicals do not naturally mix or react on their own, a catalyst is required. The precursors are mixed into an alcohol solvent to create a colloidal suspension. As the mixture is heated, the water hydrolyzes the bonds, causing the solution to thicken into a gel. DIY Doping Process Steps

* Mix the TEOS, water, and catalyst into the alcohol solvent.
* Introduce the chosen dopant atoms into the liquid suspension.
* Heat the mixture on a hot plate to partially complete the reaction and increase the viscosity. (In the recent test, this was done at 175°C, sampling the mixture every 10 minutes after an initial 20-minute heating period).
* Remove the mixture from the heat once it is viscous enough to coat evenly, but before it turns into an unspinnable solid gel.
* Spin the liquid dopant mixture onto the wafer to form a single layer.
* Anneal the wafer to drive the dopant atoms out of the glass layer and diffuse them into the silicon wafer underneath.

Current Roadblocks The main challenge with this DIY approach is controlling the variables (time, temperature, and catalyst volume) to get the perfect viscosity. If the thickness of the spun-on layer is not completely uniform, it creates visual interference colors on the wafer and can lead to inconsistent doping diffusion.


# thermal-evaporator-v1

This is the official HackerFab IITB documentation for the thermal evaporator

## The Thermal Evaporator

### Introduction: What is a Thermal Evaporator?

A thermal evaporator is a Physical Vapor Deposition (PVD) system used to deposit extremely thin films of metals (or other materials) onto a substrate. It operates inside a high-vacuum chamber.

The core principle is resistive heating: a very high electrical current is passed through a refractory metal filament (usually shaped like a basket or boat made of Tungsten or Molybdenum). The target material (like Aluminum pellets) is placed inside this filament. As the filament heats up, the metal melts and then evaporates. Because this happens in a high vacuum, the vaporized metal atoms travel in straight lines without colliding with air molecules, eventually condensing as a highly uniform thin film on the cooler substrate positioned above it.

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FfKoZgHcgxIGn8FY1n2nw%2FIMG_6167.jpg?alt=media&amp;token=2cdf050f-13c1-4463-9429-0c7b8c675aac" alt=""><figcaption></figcaption></figure>

### Disclaimer

This documentation is provided for educational and informational purposes only. Building and operating a thermal evaporator involves extreme temperatures, high electrical currents, and hazardous materials (metal vapour). By following this guide, you acknowledge that you are doing so at your own risk. The authors and HackerFab IITB are not responsible for any property damage, injury, or loss of life that may occur as a result of attempting this project. Always consult a qualified professional if you are unsure about electrical wiring or high-temperature systems. Please read the safety section carefully before proceeding.

### Specs

* Current Rating: 50 - 60 Amps
* Rotary Pump Pump-down Time (Atm to 1e-3 mbar): \~20 minutes
* Turbo Pump Pump-down Time (1e-3 to 1e-5 mbar): \~30 minutes
* Clearance (Filament to Substrate): 8.5 cm
* Evaporation Duration: 10 - 12 minutes
* Post-Process Cooling Time: 20 - 25 minutes

### Bill of Materials (BOM)

| Item                | Description/Source                               | Cost (INR)   | Type  |
| ------------------- | ------------------------------------------------ | ------------ | ----- |
| Vacuum Chamber      | Reused from Sputter v-2 build                    | N/A          | Capex |
| Rotary Pump         | Reused from Sputter v-2 build                    | N/A          | Capex |
| Turbo Pump          | Reused from Sputter v-2 build                    | N/A          | Capex |
| Pirani Gauge        | Reused from Sputter v-2 build                    | N/A          | Capex |
| Penning Gauge       | Reused from Sputter v-2 build                    | N/A          | Capex |
| Copper Feedthroughs | Custom made at RD Brothers (Khairani Road)       | \~₹ 2,000    | Capex |
| Teflon Washers      | Machined at RD Brothers (Khairani Road)          | \~₹ 1,000    | Capex |
| Gaskets             | Viton sheet machined at RD Brothers              | \~₹ 1,000    | Capex |
| Substrate Stand     | Custom machined from Stainless Steel (SS)        | \~₹ 1,000    | Capex |
| Power Supply        | Welding PSU (220V AC mains, 220A max output)     | *\[Cost?]*   | Capex |
| Electrical Gloves   | Electrically insulated; rated for at least 1000V | *\[Cost?]*   | Capex |
| Tungsten Filament   | Basket style; KMV Vacuum Technology, Bangalore   | \~₹ 900 / ea | Opex  |
| Target Metal        | e.g., Aluminum pellets (\~100 grams)             | \~₹ 2,500    | Opex  |

*\[PLACEHOLDER: Add exact model, bill link, and cost of Welding Power Supply]*&#x20;

### The Build

Note: For the primary vacuum chamber build, please refer to the Sputter v-2 documentation. The thermal evaporator uses the same chamber with modifications to accommodate high-current electrical feedthroughs.

The feedthrough design is based on the concepts shown in [this reference video](https://youtu.be/97716PkbX2M?si=dOTJ5MCQwBpCHEew).

Step-by-Step Assembly:

1. Feedthrough Preparation: Design and machine the copper feedthroughs. You also need to manufacture custom Teflon washers (for electrical isolation) and Viton gaskets (for vacuum sealing).
2. Chamber Modification: Drill two precisely spaced holes according to the length of the tungsten filament into the bottom plate of the sputter chamber to house the feedthroughs.
3. Feedthrough Installation: Install the copper feedthroughs into the bottom plate, ensuring the Viton gaskets and Teflon washers are placed correctly to maintain a tight vacuum seal and prevent electrical shorting to the steel chamber.
4. Power Connection: Connect the high-current output lines of the welding power supply securely to the external ends of the copper feedthroughs.
   * \[PLACEHOLDER: Add a picture showing the welding power supply connected to the feedthroughs]
5. Filament Installation: Inside the chamber, bridge the two copper feedthroughs using the Tungsten basket filament. Ensure the connections are tight, but do not put mechanical stress on the filament, as Tungsten is brittle.
6. Load Target Material: Place the metal evaporation pellets (e.g., Al) directly inside the Tungsten filament basket.
   * \[PLACEHOLDER: Add a picture of the pellets loaded in the basket]

### Standard Operating Procedure (SOP)

#### Phase 1: Chamber Preparation & Loading

1. Open Chamber: Take the top plate off the chamber by unscrewing the diagonally opposite screws.
2. Remove Internals: Carefully take the SS substrate stand out of the chamber.
3. Cleaning: Clean the entire internal chamber and all components that go inside (especially the substrate stand) using Acetone, followed by IPA. *Do this while wearing nitrile gloves to avoid transferring oils from your skin.*
4. Install Filament: Connect the Tungsten filament across the feedthroughs. Caution: Do not apply excessive mechanical stress to the filament, or it will snap.

   <figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2F2hkTthPWXwafrCNhAaIG%2FIMG_6163.jpg?alt=media&amp;token=d3127aef-3405-49db-a98a-43e0c1104297" alt=""><figcaption></figcaption></figure>
5. Load Pellets: Place your metal pellets inside the Tungsten filament.
6. Place Substrate: Put the SS stand back into the chamber. Place your substrate onto the stand. Double-check that the substrate is positioned perfectly over the hole in the stand, sitting at the correct height (8.5 cm) directly above the Tungsten basket. You can put a glass slide next to the silicon wafer if depositing on silicon to observe whether the deposition has started.![](https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FurVI1hovoykrPSBq8DGV%2FIMG_6172.jpg?alt=media\&token=cd47f4c3-688d-4650-b6f9-827b50188ba1)
7. Seal Chamber: Place the top plate back on and begin screwing it in.
8.

```
<figure><img src="/files/OhWuTRP54fCgqmBypkkW" alt=""><figcaption></figcaption></figure>
```

9.

```
<figure><img src="/files/WaQs9FyBc1pFK1Y47krC" alt=""><figcaption></figcaption></figure>
```

10. Connect Gauges: Connect both the Pirani gauge and the Penning gauge to their respective ports on the top plate.

#### Phase 2: Pump Down

9. Start Pirani: Turn on the Pirani gauge. The orange light will turn on, and it will read `999` (indicating atmospheric pressure).
10. Roughing Vacuum: Turn on the rotary pump. As the pump runs, firmly tighten the top plate screws to compress the O-ring and create a proper vacuum seal. The orange light on the gauge will turn off as pressure drops.
11.

```
<figure><img src="/files/33xI2MU7tEmyMrH8586B" alt=""><figcaption></figcaption></figure>
```

12. Open Turbo Valve: Wait for the rotary pump to bring the pressure down to 70-80 mbar. Once there, open the turbo valve to continue dropping the pressure.![](https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Frw8cbmnxmNO2iIUziqeB%2FIMG_6177.jpg?alt=media\&token=527a09d6-a604-4d13-86fe-e04aaa90164c)
    * \[PLACEHOLDER: Add a picture showing which valve is the turbo valve and how to open it]
13. Wait for High Vacuum Threshold: Wait approximately 20 minutes for the pressure to reach 1e-3 mbar.
14. Start High Vacuum: Turn on the Penning gauge, then turn on the turbo pump.
15. Wait for Target Vacuum: Wait roughly 30 minutes for the pressure to reach 1e-5 mbar.

Phase 3: Evaporation Process

15. Power Up (Wear 1000V rated gloves!): Turn on the welding power supply.
16. Ramp Current: Slowly ramp up the current in increments of 10 Amps at a time. Wait 30 seconds between each step to avoid thermal shock, until you reach a final current of 55 Amps.
17. Evaporate: Maintain 55 Amps for 10-12 minutes to complete the deposition process. We have observed that it takes around 6-7 minutes for the evaporation to start, probably because of the time taken to heat the tungsten and start evaporation.
18. Monitor Temperature: Periodically check the external temperature of the copper feedthroughs using a thermal gun. (Copper usually reaches only about 40°C at 55A; it is safe up to 200°C).
    * \[PLACEHOLDER: Add a picture demonstrating measuring the feedthrough temperature with the thermal gun]

#### Phase 4: Shutdown & Venting

19. Ramp Down (Wear 1000V rated gloves!): Gradually step the current down to 0 Amps, then turn off the power supply.
20. Cooling Period: Wait 25 minutes for the Tungsten filament to cool down. *Crucial:* If a hot Tungsten filament is exposed to atmospheric oxygen, it will immediately oxidize and burn out.
21. Power Down Gauges & Turbo: Turn off the Penning gauge. Turn off the turbo pump by first turning off the switch from the front and then wait for the lights on it for the speed to turn off. This takes 15 minutes. The pressure will gently rise to about 1e-4 or 1e-3 mbar.
22. Turn off turbo pump from the back.&#x20;
23. Power Down Rotary: Turn off the rotary pump. Wait roughly 20 minutes for the system to naturally vent back to atmospheric pressure.
24. Final Shutdown: Turn off the Pirani gauge and carefully remove both gauges and the MFC from the top plate.&#x20;
25. Unload: Open the top plate and take out your coated substrate!

### Safety Guidelines

As students, we tend to disregard the matter of safety under the impression *"kya hi ho jaayega?"*. However, the thermal evaporator is not a toy. Bypassing safety protocols here can result in severe injury or loss of life. We at HackerFab IITB always follow strict protocol, and you must do the same.

#### 1. Electrical Safety

The evaporator uses a welding power supply to drive 55 Amps of current through an exposed metal chassis. A simple mistake like touching the live copper feedthroughs can be fatal.

* Grounding: The chamber is made of stainless steel/mild steel and will carry leaking current. The entire enclosure must be securely grounded. Always use a multimeter to check for continuity between the chamber body and earth ground before starting the system.
* PPE (Gloves): You must wear electrically insulated gloves rated for at least 1000V whenever you are interacting with the power supply (turning it on, ramping it, or turning it off).

#### 2. High Temperature & Fire Hazards

The filament inside reaches temperatures capable of vaporizing metal, making the surrounding setup a severe fire hazard.

* Workspace Surface: Keep the evaporator on a non-combustible surface (like a concrete table, thick ceramic tiles, or a steel table).
* Clearance: Ensure there are no flammable materials, chemicals, solvents (keep the cleaning IPA/Acetone far away!), or papers within at least a 1-meter radius of the machine.
* Fire Extinguisher: Always keep a suitable fire extinguisher immediately accessible.
* Thermal Discipline (Cooling Time): Always respect the 25-minute cooling rule after evaporation before venting the chamber. Opening it while the filament is hot will destroy the filament and create a spontaneous fire/burn hazard.

#### 3. Material Handling & Chemical Hazards

* Consult the MSDS: Always check the Material Safety Data Sheet (MSDS) of the target metal before evaporating it. You might think you are playing with a harmless material, only to find out its vapour or oxide form is a toxic carcinogen!
* Hygiene: Wear nitrile gloves during the entire cleaning and loading process to avoid skin exposure to solvents, metal residues, and to prevent contaminating the vacuum chamber with organic oils from your hands.

### Thermal Evaporator V2: Planned Improvements

While the current setup is functional, the following improvements are planned for the next iteration of the evaporator to increase safety, reliability, and ease of use:

1. Dedicated Chamber: The current evaporator shares a chamber with the Sputter setup. V2 will feature a completely separate, dedicated vacuum chamber. This will allow both machines to be operated independently and simultaneously, increasing lab throughput and preventing cross-contamination between processes.
2. Turbo Pump Isolation Valve (Baffle/Flap): A high-vacuum gate valve or baffle will be installed between the turbo pump and the main chamber. This will allow the turbo pump to be closed off once the target vacuum is reached, preventing evaporated metal vapors from entering the pump, condensing on the rapidly spinning blades, and causing mechanical failure or unbalancing.
3. Thickness Monitor: Integrating a Quartz Crystal Microbalance (QCM) inside the chamber to measure the thickness of the deposited film in real-time, allowing for precise control over the final coating thickness.

{% embed url="<https://www.youtube.com/watch?v=97716PkbX2M>" %}


# Wafer Info


# Wafer Handling

## Wafer Holding

## Wafer Cleaning

## Wafer Cutting

## Wafer Storage


# Liftoff and Undercut in Deposition

TODO

Liftoff is the simplest way to create a pattern using deposition and lithography (sputtered metal in our case).

Patterned and developed photoresist blocks certain areas of the substrate and leaves the rest exposed to deposition. However, sputtering is conformal: it coats all surfaces with a non-zero film thickness, independent of deposition. Thus there would be no way to develop the photoresist as the metal deposition blocks the developer.

Undercut means creating a laterally larger hole in liftoff-resist underneath the photoresist layer. If the LOR layer is thicker than the deposition, it leaves place for the developer to attack the resists.

The developer removes the resists and the metal layer above lifts and floats away, hence the term **liftoff.**


# Litho performance

Resolution, Dose Matrix, Under/overdevelopment, characterization techniques

## Resolution test patterns

Pitch: the spacing between corresponding points of an array. Known in math as the period:

$$
T: f(x+T=f(x)
$$

A line array with 50% duty cycle is a pattern with linewidth=x, spacewidth=x, and period=x+x=2x

Isolated lines take spacewidth>>linewidth giving enough room for underexposed tails to extend

## Characterization Techniques

### Visual inspection: Optical Microscope

Gives inexpensive and immediate visual feedback: interference colours show resist thickness variation.

### Cross-section and 3D mapping: Profilometry, AFM


# MOSCAP

MOSCAPs(with shadow mask)

1. Clean
2. Oxidise 1100C for 30 mins
3. Evaporate through Al foil shadow mask with holes in it made by sewing needle or pin
4. Scratch the backside(if no HF etch capabilities) - Or Put resist on top and etch the bottom(if HF etch capable)
5. (Optional) - evaporate Al for backside contact
6. Probe each capacitor in Proxima and do the CV characterisation&#x20;

### Some runs

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FJIBJEgYak1t9x1ZoXekB%2Fimage.png?alt=media&amp;token=1cb0fd9a-329d-456d-ab88-ee6b40ef9baa" alt=""><figcaption></figcaption></figure>

{% file src="/files/5mphMdWUcAyPphVf2zTM" %}


# Diode

### SOP

### Characterized Curves

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FqicmpA5L1VzknVCEd8c8%2Fimage.png?alt=media&amp;token=50c3f2f2-988f-4091-b704-3807df8fb2c2" alt=""><figcaption></figcaption></figure>

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FsHMxpJDegJcg05du1MUV%2Fimage.png?alt=media&amp;token=600b0dce-a323-476a-a82b-fc275c85383d" alt=""><figcaption></figcaption></figure>


# Liftoff

1. 1. Solvent Clean and N2 Dry
      2\. Dehydration Bake
      3\. Cool(room temp)
      4\. Spin Coat 70uL of LOR
      5\. Final Speed - 3000 rpm
      6\. Accel/Decel - 300 rpm/s
      7\. Total Time - 50s(i.e. Time at final speed = 30s)
      8\. Bake 190C for 5 mins
      9\. Cool(room temp)
      10\. Spin Coat 70uL of S1813 PPR
      11\. Final Speed - 4000 rpm
      12\. Accel/Decel - 400 rpm/s
      13\. Total Time - 50s(i.e. Time at final speed = 30s)
      14\. Expose - big checkerboard pattern - 65s
      15\. Develop in MF319 - 60s
      16\. Sputter - 115W for 30 mins
      17\. Remove resist - Acetone/PG remover at 100C for \~5 mins

i think this misses a pre exposure bake we generally do with PPR


# NMOS

## Process Flow:

1. Field oxide growth in furnace (need to see if oxide quality is good by building MOSCAPs reliably)
2. Coat PPR
3. Litho and develop areas for source and drain
4. Bake and harden the PPR so it can survive HF
5. HF etch the oxide down to silicon in source and drain areas, remove photoresist
6. Coat spin on dopant, do the doping process as described, don't etch the field oxide- this gives visibility of S/D regions crucial for future alignment
7. Coat PPR again, align gate mask between source and drain using XY and theta stages(this will easily be done with our current setup), do the litho and development of gate
8. HF Etch oxide underneath gate region again through photoresist mask as before till it reaches the bottom
9. Remove photoresist
10. Grow a thin gate oxide(start \~100nm and play around with this number) - the etch was done so you can have control over regrowth - this thickness has a high impact on device performance
11. Coat resist for a third mask, this is the contacts walla mask- again do the same litho process- etch through to reach the Si on the source and drain for contacts using PPR as a mask
12. Now you have to actually deposit the gate and contacts metal - one option is LOR PPR, and then do the liftoff process while aligning - second option is blanket metal deposition, then etch everything but what you want after doing PPR and litho and using the PPR as a mask for Al etchant

### Sub-Processes

1. MOSCAPs through shadow mask - they confirm oxide quality

2. Etching oxide through PPR as a mask - used again and again in the process flow and a hard nut to crack.

3. Simple Big diodes - Confirm doping capabilities as well as how good the contacts are

4. Liftoff/metal etch along with lithography- basically be able to make good arbitrary patterns with metal

5. Building on 4 and 1 - build MOSCAPs at micron scale by combining

6. Building on 4 and 3 - build diodes at micron scale by combining

7. Just generally each tool owner should do runs with the tool at least every 2 days, so tools are never a bottleneck

#### Some learnings/suggestions

* Contact & Probing Improvements
  * Indium Paste: Good alternative for contacts, though harder to source.
  * Silver Epoxy: A low temperature conductive bridge suitable for larger initial devices to overcome contact issues
* Photoresist Adhesion & HF Oxide Etch Protection
  * HMDS + Dehydration + Bake: A combination of these step might help us solve the problem of HF attacking photoresist
  * Strict Humidity Control: Perform dehydration bakes and spin coating in a low humidity environment
  * Chromium (Cr) Hard Mask: Deposit a thin metal layer to act as the primary HF barrier, which can also help us with the problem of HF attacking photoresist
  * BOE(Buffered Oxide Etch) might be better for SiO2 etching

#### Some important links:

Previous moscap + diode runs : [HackerFab Characterisation - Google Docs](https://docs.google.com/document/d/1XJMAsDky3MLmV7WHJEA6A1dmiy9wwV_OrWoT6nEKNgk/edit?tab=t.0)\
Moscap lab report(from some course?) : [MOSCap Lab Report (18-410/610 S26) - Google Docs](https://docs.google.com/document/d/1vXfvOCq2npE0pBO5wzHDL6-moE2DDtNtiPALTWdSElE/edit?tab=t.0)\
Reference youtube links for process: <https://youtu.be/h6GWikWlAQA?si=-4tnxWmMNuInQbWL>(small devices)\
<https://youtu.be/s1MCi7FliVY?si=qV3K9AzkhmW9XfwS>(big devices)

RCA Cleaning: <https://youtu.be/bS4VtjRc3og?si=hjJ5zUZQisqlUsgI>\
<https://youtu.be/wL10iqP2xI8?si=rpe0rnTaM42b8SS-><br>


# Doping

## SOP:

1. Coat the dopant(check datasheet/ask claude about speed/time)
2. Bake on hot plate - excess solvent goes away - just watch videos/see online for what parameters to do it at.
3. First diffusion step
4. Etch
5. Second diffusion step
6. Etch


# HackerFab Universe

## Sam Zeloof

## Applied Science

## Huygens Optics

## Dr. Semiconductor


# Runs

A timeline of runs on our tools, with data, images and results

A run is a self-contained cycle of fabricating and characterizing. It can be a job on a single tool, like running a resolution test pattern on the litho, or a process for fabricating an entire device.

1. [2026-07-07 furnace ellipso](https://docs.hackerfabiitb.org/runs/2026-07-07-furnace-ellipso)
2. [2026-07-07 sputter profilo](https://docs.hackerfabiitb.org/runs/2026-07-07-sputter-profilo)
3. [USAF resolution test](https://docs.hackerfabiitb.org/runs/usaf-resolution-test)


# 2026-07-07 furnace ellipso

### Objective

Measure the thickness of $$SiO\_2$$ grown on a silicon sample (with native oxide) in our tube furnace at $$1100^{\circ}\text{C}$$

### Process

1. Wafer: Si, 4-inch, p-type, 100
2. Cleave wafer into 2cm x 1cm samples
3. Preheat tube furnace to $$1100^{\circ}\text{C}$$
4. Place sample inside for t minutes, t ranging from 5 to 45 in increments of 5
5. Measure thermal oxide thickness using Woollam Ellipsometer @ IITNF

### Plot

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FY7KYBbSkhLSe522nC6GN%2FPLOT.png?alt=media&amp;token=c610d17b-4212-450c-ad39-444cabf5282f" alt=""><figcaption></figcaption></figure>

### Data

{% embed url="<https://docs.google.com/spreadsheets/d/1_P1HrZYgONitlHiEv3FEB-wu93_731-pv0060k5gJcg/edit?usp=sharing>" %}


# 2026-07-07 sputter profilo

### Process

Aluminium sputter, power = 115W, duration = 5min, 15min, 30min

### Samples

#### Sample 1: 5min, 115W. 38-47nm

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2Fkcf0Dyr83jVBMLBW9FZD%2Fimage.png?alt=media&amp;token=11a8166b-6f96-4ecd-b35e-5eed034fc936" alt=""><figcaption></figcaption></figure>

comments: very dirty - black spots on both Si and deposited Al

Reading 1:

Scan length: 240um\
**Step height: 47nm**\
**Profile:**

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FBKvmASq3EeGEIGPcFlqe%2Fimage.png?alt=media&amp;token=df701482-fc64-41a8-a36f-9d52865a6a52" alt=""><figcaption></figcaption></figure>

Reading 2:

Scan length: 80um\
**Step height: 38nm**

Profile:

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2F1C55DCmfxtw8uhebncX9%2Fimage.png?alt=media&amp;token=fc104d78-5e1a-40b6-b2c6-ca54d5933dea" alt=""><figcaption></figcaption></figure>

#### Sample 2: 15min, 115W.&#x20;

Reading 1:

comments: sample was much cleaner visually

scan location:\
![](https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FyXXIHmfwGOVnC8GS3w8Q%2Fimage.png?alt=media\&token=6bd38f03-3646-42c1-b161-5b918b970904)

scan length: 325um\
scan duration: 325s\
horizontal resolution according to software: 3nm/pt

<figure><img src="https://1411217458-files.gitbook.io/~/files/v0/b/gitbook-x-prod.appspot.com/o/spaces%2FdVHY4TMcc4U7ByfYShMQ%2Fuploads%2FDOXZYalwgyhDC3cLtMBt%2Fimage.png?alt=media&amp;token=92d6abe3-eb15-4f97-b74b-fa49f48ae664" alt=""><figcaption></figcaption></figure>

step visible at 0.12mm, but no flat region on either side

after fitting two point linear:

### TODO&#x20;


# USAF resolution test